      Production Process of Carbonized wood outdoor chairs

      "Carbonized wood" gluing properties and surface finishing, good performance, and pine in the heat treatment process, turpentine basically volatile resin has cured, therefore, the resin ducts and Setsuko surface, do not do special sealing process can be directly do finishes. Carbonized wood outdoor chairs in use, it will not happen hot weather resin overflow, destroying the paint surface problems.

      Kiln and tank "carbonized wood" outdoor chair production process are divided into primary drying and secondary drying, charring rapid heating, cooling and conditioning treatment, and then cooling the kiln (tank) 5 phase.

      1 Primary Drying

      From birth (wet) wood dried to approximately 12% (or 10%) moisture phase is called once dry. This stage can be in the kiln carbonization (tank) carried, also accomplished by conventional kiln. Given carbonization kiln (tank) of the cost is higher, and the high cost of equipment operation, so using conventional drying kiln for a more economical, and the drying quality is also easier to control, but the drying time.

      (2) second drying

      From 12% dried to a wood moisture content of 3% (or 4%) of the second drying phase is called. This phase carbonization furnace (tank) to complete. Moisture content of about 12% of the timber into the carbonization kiln, the first transition can be conventional drying. Dry bulb temperature from about 65-75 ℃ Start, and then heated in stages to about 125 ℃, wet bulb temperature gradually expanded to 25 ℃. Subject wood moisture content to about 3%, the secondary drying stage ends. This phase of the length of time, depending on the wood species and thickness, 22mm thick timber normally takes more than 10 hours.

      3 rapid heating carbonization

      Wood moisture content of 3% after, they spent the dry dangerous period. Can quickly heat up, in a relatively short period of time, rising carbonization temperature (usually 180 ~ 212 ℃). Carbonization temperature then held constant for about 3 hours, high temperature heat treatment of wood, the wood of the hemicellulose and amorphous cellulose degradation, wood moisture greatly reduce the number of hydroxyl groups. Meanwhile in wood extractives such as resin, terpenoids, tannins, acids, a large number of objects containing volatile. Thus greatly reduced hygroscopicity of wood, dimensional stability and significantly improved corrosion resistance. This stage, the kiln (tank) to be filled within a protective gas (usually water vapor), oxygen gas must be less than 2%, a simple measure of the kiln to maintain the wet-bulb temperature of 99.5 ~ 100 ℃.Otherwise, there will be very dry wood fire hazard, and the wood under high temperature oxidation, its strength is also unfavorable.

      4 cooling humidity

      Wood carbonization treatment, not only the water content is very low (0.5%), and the wood itself, the temperature is high, close to 180 ~ 212 ℃. Then the humidity can not be directly processed must first timber to cool. Note do not use air cooling, if the kiln outside in the fresh air flow into the kiln, it is easy to make wood fire. The correct way is to stop the radiator heating while spraying atomized water to the kiln, not only play a role in cooling, but also make almost all dry timber proper humidification.Subject to the kiln medium temperature dropped about 116 ℃, humidity conditioning treatment can be carried out. Then the kiln while the saturated water vapor injection, and then atomized water spray in order to enhance the relative humidity of the kiln medium moisture content of wood, and to eliminate the residual stress. Wood moisture content generally be increased from 4 to 5%, to end the humidity treatment.

      聯系我們

      聯系人:陳先生

      手機:13521257486

      電話:010-82921102

      郵箱:zhitong_chenfei@163.com

      地址: 北京市海淀區(qū)

      主站蜘蛛池模板: 99国精品午夜福利视频不卡| 日本高清不卡码| 色婷婷综合久久久久中文一区二区| 少妇人妻久久无码专区| 国产精品免费电影| 黄色片网站免费看| 1000部啪啪未满十八勿入下载| 亚洲国产成人av片在线播放| 国产第十页| 欧美激情第三页| 久久av一区二区三区| 丰满少妇呻吟高潮经历| 操天天| 九九影院最新理论片| 一本一道精品欧美中文字幕| 最新av偷拍av偷窥av网站| 综合久久av| 欧美色欧美| 人妻少妇偷人精品视频| 国产美女精品视频线免费播放软件| 欧美黄色三级| xxx精品| 免费网站观看www在线观看| 国产偷伦视频片免费视频| 成人动态视频| 2020国产精品视频| 亚洲精品不卡无码福利在线观看| 午夜亚洲影院在线观看| 先锋影音资源av| 男女涩涩网站| 国产一区二区三区乱码| 色悠久久久久综合欧美99| 亚洲男人的天堂av| 美女久久视频| 国产精品无遮挡猛进猛出| 在线麻豆精东9制片厂av影现网| 国产高清一区| 国产精品一区二区三区四区在线观看 | youjizzxxxxx| 九九小视频| 免费看成人欧美片爱潮app|